CuZn37 / C27400
|
US Customary |
Metric |
| Melting Point - Liquidus |
1680 F |
916 C |
| Density |
0.305 lb/in3 at 68 F |
8.44 gm/cm3 @ 20 C |
| Specific Gravity |
8.44 |
8.44 |
| Electrical Conductivity |
27 %IACS @ 68 F |
0.161 MegaSiemens/cm @ 20 C |
| Thermal Conductivity |
67.0 Btu · ft/(hr · ft2·oF)at 68F |
116.0 W/m · oK at 20 C |
| Coefficient of Thermal Expansion |
11.4 ·10-6 per oF (68-572 F) |
20.5 ·10-6 per oC (20-300 C) |
| Specific Heat Capacity |
0.09 Btu/lb/oF at 68 F |
377.1 J/kg · oK at 293 K |
| Modulas of Elasticity in Tension |
15000 ksi |
103400 MPa |
| Modulas of Rigidity |
6400 ksi |
44130 MPa |
Blanking, Drawing, Forming and Bending, Roll Threading and Knurling, Shearing, Spinning, Squeezing and Swaging, Stamping
| Joining Technique |
Suitability |
| Soldering |
Excellent |
| Brazing |
Excellent |
| Oxyacetylene Welding |
Good |
| Gas Shielded Arc Welding |
Fair |
| Coated Metal Arc Welding |
Not Recommended |
| Spot Weld |
Good |
| Seam Weld |
Not Recommended |
| Butt Weld |
Good |
| Capacity for Being Cold Worked |
Excellent |
| Capacity for Being Hot Formed |
Fair |
| Machinability Rating |
35 |
|